Welding Standards
DIN 8555
RSS
Classification of coated rod electrodes for arc welding of unalloyed steel and fine-grained steel
Example Garant
E
1
42
2
2
3
B
5
4
6
2
7
H10
8
Young Welders in
Finsterwalde
In the National
Competition the Kjellberg
electrode Titan was used
Code number
Minimum
yield strength*1
Re (N/mm2 )
Tensile strength
Rm (N/mm2 )
Minimum elongation
after fracture A5 (%)
35
355
440 - 570
22
38
380
470 - 600
20
42
420
500 - 640
20
46
460
530 - 680
20
50
500
560 - 720
18
Aquaweld Certified up
to 20 m Water Depth
First Rod Electrode for
Underwater Welding
*1 Yield strength should be the lower yield point R. If it is not distinct then choose the 0.2 % yield strength R.
none
+20
-20
-30
-40
-50
-60
Successful in
Competition for
Juvenile Welders
The Kjellberger Stefan
Richter wins the MMA
Welding Competition
Chemical composition
Mn
Mo
Ni
no short symbol
2.0
Mo
1.4
0.3 - 0.6
Mn Mo
> 1.4-2.0
0.3 - 0.6
1 Ni
1.4
0.6 - 1.2
2 Ni
1.4
1.8 - 2.6
3 Ni
1.4
2.6 - 3.8
Mn 1 Ni
> 1.4-2.0
0.6 - 1.2
1 Ni Mo
1.4
0.3 - 0.6
0.6 - 1.2
*2 if not determined: Mo<0.2; Ni<0.3; Cr<0.2; V<0.08; Nb<0.05; Cu<0.3; individual values are
maximum values
Short symbol
Coating type
acid
cellulose
rutile
RR
heavy-rutile *3
RC
rutile-cellulose
RA
rutile-acid
http://www.kjellberg.de/Electrodes-de-soudage/Service/Normes/DIN-EN-ISO-2560-...
09-12-2015
RB
rutile-basic
basic
Pgina 2 de 2
Short symbol
Recovery (%)
<105
AC, DC
<105
DC
>105 - 125
AC, DC
>105 - 125
DC
>125 - 160
AC, DC
>125 - 160
DC
>160
AC, DC
>160
DC
Short symbol
Code
Type of current
Welding position
all positions
H5
H10
10
H15
15
http://www.kjellberg.de/Electrodes-de-soudage/Service/Normes/DIN-EN-ISO-2560-...