z Welding of Thermoplastics, Direction
orTOR SCHWEISSEN UND Extrusion Welding DVS 2207-4
Panels and Pipes, Supplement
\VERWANOTE VERFAHREN E-. Welding Parameters for HDPE and PP (duly 1999)
“This eupplement provides guideline values forthe extrusion welding of HOPE and PP.
‘Material thickness”) | Material Hota ‘ir ate®) Wielding filer rate
(lor single-pass welding) | temperature? | temperature
ram "c [rc Vein kon
Continuous process with
‘manual equipment (screw)
Process valant
Continuous process with
‘welding filer transfer hose
between exruder and welding
head 230 | 260...900 | 2300
Process variant I 230 | 260... 300 00
Continuous process with
manual equipment (cam) Figures silt be released
Process vavant V
Discontinuous process wih
‘manual transte ofthe welding
filer into the preheated wel
‘ding groove 200.290 | 250..300 | »900
Procass variant
‘The parameters of ot air temperature, lr rate and welding speed must be coordinated in such a way thatthe minimum depth of
‘making required in Clause 8 of 0.5 mms defintely ensured
7 Tike atoralis tobe welded, wel wth mexe than ene pass.
2 Measure wih a penetration teometr atthe extutate ou othe welding exude.
3) Measured between he pane of nozle out and mm inside the nazz.
Cold ai takann at abou 20°C an etmospherc pressure in the operational slat. supp tom pressurized ai sytoms, the ar pressure shal
‘Semessurod downsronm oe ait meter an slowance mage for hs y a peste or rat Srwersin,
“Thi pulation mas bean dawn wp grup ol epee speci wring in an near capa and cin i commend. The ua sould
“hays chest oat ene cntata ste apical lohispartclrease ard whether wren hana cl va The Deus Vasa Schetechk
£287Sed hes imed rapeng hs puesto ate exer Wom an ai
DVS, Technical Committee, Working Group “Plastics, Welding and Bonding
‘Orders to: BVS-erag GmbH, PO Bax 101965, 40010 Dusseldr, Germany, Phone +49(0}21/1601-0, Tlf +49(0)211159-150,