Вы находитесь на странице: 1из 19

Contract / Job No.

:
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1250
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : 23 October 2017 IQI : ASTM 1B
Material : SS Technique Details : DWSI Min. SOD : 10 Inch Kv / mA : -
Radiation Source : Ir-192 Max. SSOD to Film : 12.7 mm Curie : 23.50 Ci
Welding Process : GTAW,SMAW Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : 4x15 Inch Exposure Time : 1 Min 23 Sec
Request for Inspection (RFI) No.: N/A
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Sensitivity (%)

Surface Defect
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Film Position

Discontinuity
Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

Porosity
No Sign
Density

Crack
(mm)
Joint

ACC

REJ
Drawing / Spool Number
Number

### 1 A220_HG31003 013 0 - 11 10'' 12.70 SWG-09 2.7-2.9 1.5 √ √ Root UC


### 11 - 22 2.7-3.1 √ √
### 22 - 0 2.7-2.9 √ √
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
Radiographer : Verified and Interpreter : Subcontractor (Swadaya) : Contractor (JEC) : Company (Medco) :

Name: Bastari P. Name: Ahmat


Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date23 October 2017 Date : Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1251
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : 23 October 2017 IQI : ASTM 1B
Material : SS Technique Details : DWSI Min. SOD : 10 Inch Kv / mA : -
Radiation Source : Ir-192 Max. SSOD to Film : 12.7 mm Curie : 23.50 Ci
Welding Process : GTAW,SMAW Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : 4x15 Inch Exposure Time : 1 Min 23 Sec
Request for Inspection (RFI) No.: N/A
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

### 1 A620_HG32003 007 0 - 11 10'' 12.70 SWG-09 2.7-3.0 1.5 √ √


### 11 - 22 3.0-3.2 √ √
### 22 - 0 2.8-3.1 √ √
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
Radiographer : Verified and Interpreter : Subcontractor (Swadaya) : Contractor (JEC) Company (Medco)

Name: Bastari P. Name: Ahmat

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date23 October 2017 Date : 23 October 2017 Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1252
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : 23 October 2017 IQI : ASTM 1A
Material : LTCS Technique Details : DWSI Min. SOD : 10 Inch Kv / mA : -
Radiation Source : Ir-192 Max. SSOD to Film : 6.35 mm Curie : 23.50 Ci
Welding Process : GTAW,SMAW Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : 4x15 Inch Exposure Time : 47 Seconds
Request for Inspection (RFI) No.: RTQ-JEC-0210
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

### 1 A310_FL47021 009 0 - 11 10'' 6.35 SWG-17 2.3-2.8 1.1 √ √ √ C.Por L=5 mm & EP
### 11 - 22 2.4-2.8 √ √
### 22 - 0 2.5-2.8 √ √ Por Ø < 1 mm
###
### 2 A310_FL47021 013 0 - 11 10'' 6.35 SWG-17 2.6-3.0 1.1 √ Elongated 10 mm
### 11 - 22 2.5-2.7 √ √
### 22 - 0 2.8-3.0 √ √ HI-LOW
###
###
###
###
###
###
###
###
###
###
###
###
###
###
Radiographer : Verified and Interpreter : Subcontractor (Swadaya) : Contractor (JEC) Company (Medco)

Name: Bastari P. Name: Ahmat

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date23 October 2017 Date : 23 October 2017 Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1253
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : 23 October 2017 IQI : ASTM 1A
Material : SS Technique Details : DWSI Min. SOD : 12 Inch Kv / mA : -
Radiation Source : Ir-192 Max. SSOD to Film : 4.57 mm Curie : 23.50 Ci
Welding Process : GTAW Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : 4x15 Inch Exposure Time : 59 Seconds
Request for Inspection (RFI) No.: N/A
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

### 1 A110_HF39001 030 0 - 10 12'' 4.57 SWG-07 2.7-3.0 1.3 √ √


### 10 - 20 2.5-2.7 √ √
### 20 - 30 3.0-3.1 √ √ Por Ø < 1 mm
### 30 - 0 2.7-3.1 √ √ Por Ø < 1 mm
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
Radiographer : Verified and Interpreter : Subcontractor (Swadaya) : Contractor (JEC) Company (Medco)

Name: Bastari P. Name: Ahmat

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date23 October 2017 Date : 23 October 2017 Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1254
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : 23 October 2017 IQI : ASTM 1A
Material : SS Technique Details : DWSI Min. SOD : 16 Inch Kv / mA : -
Radiation Source : Ir-192 Max. SSOD to Film : 4.78 mm Curie : 23.50 Ci
Welding Process : GTAW,SMAW Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : 4x15 Inch Exposure Time : 1 Min 47 Sec
Request for Inspection (RFI) No.: N/A
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

### 1 A620_AM32031 001 0 - 12 16'' 4.78 SWG-01 2.5-2.6 1.3 √ √


### 12 - 24 3.1-3.2 √ √
### 24 - 36 2.8-3.1 √ √
### 36 - 48 2.9-3.0 √ √
### 48 - 0 √
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
Radiographer : Verified and Interpreter : Subcontractor (Swadaya) : Contractor (JEC) Company (Medco)

Name: Bastari P. Name: Ahmat

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date23 October 2017 Date : 23 October 2017 Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1255
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : 23 October 2017 IQI : ASTM 1B
Material : LTCS Technique Details : DWSI Min. SOD : 18 Inch Kv / mA : -
Radiation Source : Ir-192 Max. SSOD to Film : 7.92 mm Curie : 23.50 Ci
Welding Process : GTAW,SMAW Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : 4x15 Inch Exposure Time : 2 Min 57 Sec
Request for Inspection (RFI) No.: RTQ-JEC-0212
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

### 1 D310_FL47010 028 0 - 12 18'' 7.92 IT-09 2.8-3.1 1.2 √ Rounded Ø 2 mm


### 12 - 24 2.7-3.0 √ √ Por Ø< 1 mm
### 24 - 36 2.4-2.7 √ √
### 36 - 48 2.4-2.7 √ √
### 48 - 0 2.8-3.3 √ √
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
###
Radiographer : Verified and Interpreter : Subcontractor (Isma Tiur) : Contractor (JEC) Company (Medco)

Name: Bastari P. Name: Ahmat

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date23 October 2017 Date : 23 October 2017 Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1256
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : IQI : #N/A
Material : Technique Details : ### Min. SOD : Kv / mA : -
Radiation Source : Max. SSOD to Film : #N/A Curie :
Welding Process : Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : Exposure Time : #N/A
Request for Inspection (RFI) No.:
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
Radiographer : Verified and Interpreter : #N/A Contractor (JEC) Company (Medco)

### ###

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date Date : Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1257
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : IQI : #N/A
Material : Technique Details : ### Min. SOD : Kv / mA : -
Radiation Source : Max. SSOD to Film : #N/A Curie :
Welding Process : Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : Exposure Time : #N/A
Request for Inspection (RFI) No.:
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
Radiographer : Verified and Interpreter : #N/A Contractor (JEC) Company (Medco)

### ###

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date Date : Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1258
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : IQI : #N/A
Material : Technique Details : ### Min. SOD : Kv / mA : -
Radiation Source : Max. SSOD to Film : #N/A Curie :
Welding Process : Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : Exposure Time : #N/A
Request for Inspection (RFI) No.:
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
Radiographer : Verified and Interpreter : #N/A Contractor (JEC) Company (Medco)

### ###

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date Date : Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1
Contract / Job No. :
RADIOGRAPHIC INSPECTION REPORT 0-0709-0-P-3154-001-A

Report No:
CLIENT : PT. JGC INDONESIA - ENCONA INTI INDUSTRI CONSORTIUM PROJECT : BLOCK A GAS DEVELOPMENT PROJECT ACEH
TNDT-CPP-PIP-RT-1259
SPECIFICATION: ACCEPTANCE CRITERIA: PROCEDURE NO :
ASME V Article 2 ASME B31.3 BLA-C-IP-00-000-NDT-504
LOCATION: RADIOGRAPHY DATA:
Test Date : IQI : #N/A
Material : Technique Details : ### Min. SOD : Kv / mA : -
Radiation Source : Max. SSOD to Film : #N/A Curie :
Welding Process : Intensifying Screens : Pb 0.125 mm Diagnostic Film Length : Exposure Time : #N/A
Request for Inspection (RFI) No.:
WELD JOINT DETAILS WELD EVALUATION RESULTS

Tungsten Inclusion
Excess Penetration
Mat'l Thickness

Root Concavity

Lack of Fusion
Surface Defect
Sensitivity (%)
Film No.

Pipe Diameter

Slag Inclusion

Burn Thourgh
Misalignment
Discontinuity
Film Position

Welder No.

Penetration
Incomplete

Wormhole
Undercut
REMARKS

No Sign

Porosity
Density

Crack
Joint

(mm)

ACC

REJ
Drawing / Spool Number
Number

###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
### ###
###
Radiographer : Verified and Interpreter : #N/A Contractor (JEC) Company (Medco)

### ###

TNDT-JGC-FRM-RT-003 / REV:1
Qualification : BATAN OR Qualification : BATAN AR Name: Name: Name:
Date Date : Date : Date : Date :

TNDT-JGC-FRM-RT-003 / REV:1