Вы находитесь на странице: 1из 108

FISH TOWN - HARPER ROAD PROJECT PHASE 1

Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town


(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

14-Jul-17 21-Jul-17 C30 90 15 7870 2.332 727.6 32.3


PIPE CULVERT
15 7750 2.296 722.1 32.1

15 7860 2.329 679.3 30.2


TOE & APRON
11-Aug-17 15 7880 2.335 872.6 38.8

(16KM) KM 15 7770 2.302 871.3 38.7


10+311
15 7870 2.332 814.3 36.2

AVERAGE ( COMPRESSIVE STRENGTH ) 31.5 37.9

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Jul-17 25-Jul-17 C30 90 15 7960 2.359 693.8 30.8


PIPE CULVERT
15 8000 2.370 719.9 32.0

15 8026 2.378 757.2 33.7


HEAD WALL
15-Aug-17 15 7970 2.361 672.7 29.9

(16KM) KM 15 7985 2.366 711.2 31.6


10+311
15 8005 2.372 874.1 38.8

AVERAGE ( COMPRESSIVE STRENGTH ) 32.2 33.5

Remarks:

FISH TOWN - HARPER ROAD PROJECT PHASE 1


Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Contractor's Materials Engineer Checked By Materials Engineer

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Jul-17 25-Jul-17 C30 90 15 7960 2.359 693.8 30.8


PIPE CULVERT
15 8000 2.370 719.9 32.0

15 8026 2.378 757.2 33.7


WING WALL
15-Aug-17 15 7970 2.361 672.7 29.9

(16KM) KM 15 7985 2.366 711.2 31.6


10+311
15 8005 2.372 874.1 38.8

AVERAGE ( COMPRESSIVE STRENGTH ) 32.2 33.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

14-Jul-17 21-Jul-17 C30 75 15 7870 2.332 673.0 29.9


PIPE CULVERT
15 7880 2.335 652.9 29.0

15 7870 2.332 619.0 27.5


TOE & APRON
11-Aug-17 15 7865 2.330 712.7 31.7

(16KM) KM 15 7885 2.336 731.9 32.5


10+461 LHS
15 7850 2.326 733.4 32.6

AVERAGE ( COMPRESSIVE STRENGTH ) 28.8 32.3

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Jul-17 25-Jul-17 C30 90 15 7960 2.359 693.8 30.8


PIPE CULVERT
15 8000 2.370 719.9 32.0

15 8026 2.378 757.2 33.7


WING WALL
15-Aug-17 15 7970 2.361 672.7 29.9

(16KM) KM 15 7985 2.366 711.2 31.6


10+461 LHS
15 8005 2.372 874.1 38.8

AVERAGE ( COMPRESSIVE STRENGTH ) 32.2 33.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Jul-17 25-Jul-17 C30 90 15 7960 2.359 693.8 30.8


PIPE CULVERT
15 8000 2.370 719.9 32.0

15 8026 2.378 757.2 33.7


HEAD WALL
15-Aug-17 15 7970 2.361 672.7 29.9

(16KM) KM 15 7985 2.366 711.2 31.6


10+461 RHS
704
15 8005 2.372 874.1 38.8

AVERAGE ( COMPRESSIVE STRENGTH ) 32.2 33.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Jul-17 25-Jul-17 C30 120 15 7870 2.332 658.3 29.3


PIPE CULVERT
15 7980 2.364 642.9 28.6

15 7910 2.344 661.9 29.4


TOE & APRON
15-Aug-17 15 7880 2.335 710.3 31.6

(16KM) KM 15 7875 2.333 772.3 34.3


10+780
704
15 7885 2.336 731.9 32.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.1 32.8

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

3-Aug-17 10-Aug-17 C30 90 15 7925 2.348 676.3 30.1


PIPE CULVERT
15 7920 2.347 648.6 28.8

15 7940 2.353 683.1 30.4


HEAD WALL
31-Aug-17 15 7860 2.329 610.7 27.1

(16KM) KM 15 7815 2.316 721.8 32.1


10+780
704
15 7975 2.363 888.1 39.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 32.9

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Jul-17 25-Jul-17 C30 80 15 7900 2.341 651.9 29.0


PIPE CULVERT
15 7912 2.344 668.9 29.7

15 7880 2.335 681.2 30.3


TOE & APRON
15-Aug-17 15 7900 2.341 733.7 32.6

(16KM) KM 15 7950 2.356 745.3 33.1


10+955 LHS
704
15 7910 2.344 755.9 33.6

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 33.1

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

3-Aug-17 10-Aug-17 C30 90 15 7925 2.348 676.3 30.1


PIPE CULVERT
15 7920 2.347 648.6 28.8

15 7940 2.353 683.1 30.4


HEAD WALL
31-Aug-17 15 7860 2.329 610.7 27.1

(16KM) KM 15 7815 2.316 721.8 32.1


10+955 LHS
704
15 7975 2.363 888.1 39.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 32.9

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

15-Jul-17 22-Jul-17 C30 90 15 7925 2.348 676.3 30.1


PIPE CULVERT
15 7920 2.347 648.6 28.8

15 7940 2.353 683.1 30.4


PIPE SUROUND
12-Aug-17 15 7550 2.237 738.0 32.8

(16KM) KM 15 7655 2.268 715.0 31.8


11+157 LHS
15 7725 2.289 773.4 34.4

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 33.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

15-Jul-17 22-Jul-17 C30 90 15 7627 2.260 494.0 22.0


PIPE CULVERT
15 7680 2.276 471.7 21.0

15 7794 2.309 437.5 19.4


PIPE SURROUND
12-Aug-17 15 7690 2.279 569.9 25.3

(16KM) KM 15 7795 2.310 627.5 27.9


11+500 LHS
15 7755 2.298 612.8 27.2

AVERAGE ( COMPRESSIVE STRENGTH ) 20.8 26.8

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

15-Jul-17 22-Jul-17 C15 120 15 7676 2.274 841.4 37.4


PIPE CULVERT
15 7777 2.304 830.4 36.9

15 7860 2.329 814.8 36.2


BLINDING
12-Aug-17 15 8030 2.379 997.9 44.4

(16KM) KM 15 8100 2.400 1019.1 45.3


11+396 LHS
15 7970 2.361 1088.0 48.4

AVERAGE ( COMPRESSIVE STRENGTH ) 36.8 46.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

15-Jul-17 22-Jul-17 C30 120 15 7676 2.274 841.4 37.4


PIPE CULVERT
15 7777 2.304 830.4 36.9

15 7860 2.329 814.8 36.2


BASE
12-Aug-17 15 8030 2.379 997.9 44.4

(16KM) KM 15 8100 2.400 1019.1 45.3


11+396 LHS
15 7970 2.361 1088.0 48.4

AVERAGE ( COMPRESSIVE STRENGTH ) 36.8 46.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

20-Jul-17 27-Jul-17 C20 100 15 8000 2.370 606.5 27.0


PIPE CULVERT
15 7950 2.356 609.1 27.1

15 8075 2.393 593.7 26.4


PIPE SURROUND
17-Aug-17 15 7863 2.330 716.6 31.8

(16KM) KM 15 7896 2.340 704.2 31.3


11+396 LHS
15 7903 2.342 712.2 31.7

AVERAGE ( COMPRESSIVE STRENGTH ) 26.8 31.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

20-Jul-17 27-Jul-17 C20 100 15 7898 2.340 715.4 31.8


PIPE CULVERT
15 7895 2.339 705.4 31.4

15 7926 2.348 715.3 31.8


PIPE SURROUND
17-Aug-17 15 7993 2.368 843.9 37.5

(16KM) KM 15 8063 2.389 908.0 40.4


11+396 LHS
15 8100 2.400 907.0 40.3

AVERAGE ( COMPRESSIVE STRENGTH ) 31.6 39.4

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

3-Aug-17 10-Aug-17 C30 90 15 7925 2.348 676.3 30.1


PIPE CULVERT
15 7920 2.347 648.6 28.8

15 7940 2.353 683.1 30.4


HEAD WALL
31-Aug-17 15 7860 2.329 610.7 27.1

(16KM) KM 15 7815 2.316 721.8 32.1


11+396 LHS
15 7975 2.363 888.1 39.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 32.9

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

17-Jul-17 24-Jul-17 C20 70 15 7870 2.332 489.8 21.8


PIPE CULVERT
15 7780 2.305 512.8 22.8

15 7880 2.335 531.5 23.6


PIPE SURROUND
14-Aug-17 15 7985 2.366 591.5 26.3

(16KM) KM 15 7900 2.341 587.3 26.1


11+500 LHS
15 7880 2.335 558.3 24.8

AVERAGE ( COMPRESSIVE STRENGTH ) 22.7 25.7

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

3-Aug-17 10-Aug-17 C30 90 15 7925 2.348 676.3 30.1


PIPE CULVERT
15 7920 2.347 648.6 28.8

15 7940 2.353 683.1 30.4


WING WALL
31-Aug-17 15 7860 2.329 610.7 27.1

(16KM) KM 15 7815 2.316 721.8 32.1


11+500 LHS
15 7975 2.363 888.1 39.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 32.9

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

17-Jul-17 24-Jul-17 C15 70 15 7700 2.281 707.8 31.5


PIPE CULVERT
15 7720 2.287 727.2 32.3

15 7720 2.287 704.1 31.3


BLINDING
14-Aug-17 15 7997 2.369 966.2 42.9

(16KM) KM 15 8037 2.381 755.0 33.6


11+697 LHS
15 7866 2.331 965.1 42.9

AVERAGE ( COMPRESSIVE STRENGTH ) 31.7 39.8

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

17-Jul-17 24-Jul-17 C30 70 15 7700 2.281 607.8 27.0


PIPE CULVERT
15 7720 2.287 527.2 23.4

15 7720 2.287 604.1 26.8


BASE
14-Aug-17 15 7863 2.330 654.2 29.1

(16KM) KM 15 7896 2.340 759.5 33.8


11+697 LHS
15 7903 2.342 679.4 30.2

AVERAGE ( COMPRESSIVE STRENGTH ) 25.8 31.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

22-Jul-17 29-Jul-17 C30 100 15 8100 2.400 688.5 30.6


PIPE CULVERT
15 8005 2.372 710.2 31.6

15 7887 2.337 730.2 32.5


TOE & APRON
19-Aug-17 15 7810 2.314 788.2 35.0

(16KM) KM 15 7870 2.332 767.2 34.1


11+697 LHS
15 7900 2.341 780.2 34.7

AVERAGE ( COMPRESSIVE STRENGTH ) 31.5 34.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

22-Jul-17 29-Jul-17 C20 80 15 7870 2.332 576.9 25.6


PIPE CULVERT
15 7880 2.335 572.7 25.5

15 7890 2.338 590.2 26.2


PIPE SURROUND
19-Aug-17 15 7720 2.287 617.7 27.5

(16KM) KM 15 7720 2.287 596.3 26.5


11+697 LHS
15 7765 2.301 625.2 27.8

AVERAGE ( COMPRESSIVE STRENGTH ) 25.8 27.2

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

22-Jul-17 29-Jul-17 C20 75 15 7870 2.332 560.1 24.9


PIPE CULVERT
15 7880 2.335 557.4 24.8

15 7980 2.364 592.7 26.3


PIPE SURROUND
19-Aug-17 15 7940 2.353 619.2 27.5

(16KM) KM 15 7790 2.308 598.6 26.6


11+697 LHS
15 7880 2.335 624.6 27.8

AVERAGE ( COMPRESSIVE STRENGTH ) 25.3 27.3

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

3-Aug-17 10-Aug-17 C30 90 15 7925 2.348 676.3 30.1


PIPE CULVERT
15 7920 2.347 648.6 28.8

15 7940 2.353 683.1 30.4


WING WALL
31-Aug-17 15 7860 2.329 610.7 27.1

(16KM) KM 15 7815 2.316 721.8 32.1


11+697 LHS
15 7975 2.363 888.1 39.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 32.9

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

20-Jul-17 27-Jul-17 C15 170 15 7930 2.350 780.0 34.7


PIPE CULVERT
15 7985 2.366 535.6 23.8

15 7813 2.315 630.0 28.0


BLINDING
17-Aug-17 15 8044 2.383 724.6 32.2

(16KM) KM 15 8050 2.385 686.4 30.5


11+939 LHS
15 7684 2.277 814.5 36.2

AVERAGE ( COMPRESSIVE STRENGTH ) 28.8 33.0

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

20-Jul-17 27-Jul-17 C30 170 15 7930 2.350 780.0 34.7


PIPE CULVERT
15 7985 2.366 535.6 23.8

15 7813 2.315 630.0 28.0


BASE
17-Aug-17 15 8044 2.383 724.6 32.2

(16KM) KM 15 8050 2.385 686.4 30.5


11+939 LHS
15 7684 2.277 814.5 36.2

AVERAGE ( COMPRESSIVE STRENGTH ) 28.8 33.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

24-Jul-17 31-Jul-17 C20 170 15 8130 2.409 613.1 27.2


PIPE CULVERT
15 7990 2.367 670.2 29.8

15 8060 2.388 580.2 25.8


PIPE SURROUND
21-Aug-17 15 8065 2.390 703.7 31.3

(16KM) KM 15 31260 9.262 679.8 30.2


11+939 LHS
15 8130 2.409 699.6 31.1

AVERAGE ( COMPRESSIVE STRENGTH ) 27.6 30.9

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

24-Jul-17 31-Jul-17 C20 125 15 7780 2.305 598.3 26.6


PIPE CULVERT
15 7975 2.363 556.7 24.7

15 7770 2.302 580.4 25.8


PIPE SURROUND
21-Aug-17 15 7980 2.364 603.2 26.8

(16KM) KM 15 7880 2.335 673.7 29.9


13+936 LHS
15 7870 2.332 648.3 28.8

AVERAGE ( COMPRESSIVE STRENGTH ) 25.7 28.5

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

24-Jul-17 31-Jul-17 C30 125 15 777 0.230 687.4 30.6


PIPE CULVERT
15 7775 2.304 664.9 29.6

15 7780 2.305 660.7 29.4


PIPE SURROUND
21-Aug-17 15 8001 2.371 756.9 33.6

(16KM) KM 15 8015 2.375 752.0 33.4


13+936 LHS
15 7885 2.336 798.4 35.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.8 34.2

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

3-Aug-17 10-Aug-17 C30 90 15 7925 2.348 676.3 30.1


PIPE CULVERT
15 7920 2.347 648.6 28.8

15 7940 2.353 683.1 30.4


WING WALL
31-Aug-17 15 7860 2.329 610.7 27.1

(16KM) KM 15 7815 2.316 721.8 32.1


11+939 LHS
15 7975 2.363 888.1 39.5

AVERAGE ( COMPRESSIVE STRENGTH ) 29.7 32.9

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

30-Jul-17 6-Aug-17 C30 100 15 8100 2.400 688.5 30.6


PIPE CULVERT
15 8005 2.372 710.2 31.6

15 7887 2.337 730.2 32.5


PIPE SURROUND
27-Aug-17 15 7810 2.314 788.2 35.0

(16KM) KM 15 7870 2.332 767.2 34.1


12+489 RHS
15 7900 2.341 780.2 34.7

AVERAGE ( COMPRESSIVE STRENGTH ) 31.5 34.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

30-Jul-17 6-Aug-17 C20 110 15 8205 2.431 701.8 31.2


PIPE CULVERT
15 8160 2.418 586.9 26.1

15 8080 2.394 605.1 26.9


PIPE SURROUND
27-Aug-17 15 8105 2.401 702.2 31.2

(16KM) KM 15 8190 2.427 713.7 31.7


12+489 RHS
15 8185 2.425 750.9 33.4

AVERAGE ( COMPRESSIVE STRENGTH ) 28.1 32.1

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer

FISH TOWN - HARPER ROAD PROJECT PHASE 1


Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

30-Jul-17 6-Aug-17 C20 90 15 8035 2.381 654.2 29.1


PIPE CULVERT
15 7955 2.357 625.2 27.8

15 7810 2.314 582.1 25.9


PIPE SURROUND
27-Aug-17 15 7980 2.364 745.0 33.1

(16KM) KM 15 7930 2.350 689.7 30.7


12+489 RHS
15 7967 2.361 630.4 28.0

AVERAGE ( COMPRESSIVE STRENGTH ) 27.6 30.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

22-Jul-17 29-Jul-17 C15 120 15 7900 2.341 693.7 30.8


PIPE CULVERT
15 7930 2.350 644.1 28.6

15 8000 2.370 654.1 29.1


PIPE SURROUND
19-Aug-17 15 8000 2.370 901.3 40.1

(16KM) KM 15 7775 2.304 856.8 38.1


12+489 RHS
15 7900 2.341 877.0 39.0

AVERAGE ( COMPRESSIVE STRENGTH ) 29.5 39.0

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

8-Aug-17 15-Aug-17 C20 130 15 7180 2.127 573.1 25.5


PIPE CULVERT
15 7880 2.335 621.4 27.6

15 7715 2.286 565.9 25.2


PIPE SURROUND
5-Sep-17 15 7825 2.319 696.1 30.9

(16KM) KM 15 8015 2.375 652.5 29.0


13+028 LHS
15 7915 2.345 679.1 30.2

AVERAGE ( COMPRESSIVE STRENGTH ) 26.1 30.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

7-Aug-17 14-Aug-17 C20 190 15 7815 2.316 564.3 25.1


PIPE CULVERT
15 7960 2.359 578.0 25.7

15 7905 2.342 520.1 23.1


PIPE SURROUND
4-Sep-17 15 7973 2.362 625.3 27.8

(16KM) KM 15 8080 2.394 662.8 29.5


13+028 LHS
15 7930 2.350 682.2 30.3

AVERAGE ( COMPRESSIVE STRENGTH ) 24.6 29.2

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

1-Aug-17 8-Aug-17 C15 70 15 7925 2.348 664.7 29.5


PIPE CULVERT
15 7990 2.367 523.8 23.3

15 7915 2.345 711.1 31.6


BLINDING
29-Aug-17 15 7825 2.319 763.9 34.0

(16KM) KM 15 7940 2.353 680.6 30.2


13+028 RHS
15 7965 2.360 781.7 34.7

AVERAGE ( COMPRESSIVE STRENGTH ) 28.1 33.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

1-Aug-17 8-Aug-17 C30 70 15 7965 2.360 641.6 28.5


PIPE CULVERT
15 7970 2.361 656.1 29.2

15 7965 2.360 690.3 30.7


BASE
29-Aug-17 15 8025 2.378 778.6 34.6

(16KM) KM 15 8140 2.412 753.0 33.5


13+028 RHS
15 8020 2.376 781.3 34.7

AVERAGE ( COMPRESSIVE STRENGTH ) 29.5 34.3

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

5-Aug-17 12-Aug-17 C30 80 15 7895 2.339 737.1 32.8


PIPE CULVERT
15 7865 2.330 674.0 30.0

15 7925 2.348 602.4 26.8


TOE & APRON
2-Sep-17 15 8080 2.394 883.5 39.3

(16KM) KM 15 7890 2.338 831.1 36.9


13+028 RHS
15 7925 2.348 881.1 39.2

AVERAGE ( COMPRESSIVE STRENGTH ) 29.8 38.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

8-Aug-17 15-Aug-17 C20 130 15 7180 2.127 573.1 25.5


PIPE CULVERT
15 7880 2.335 621.4 27.6

15 7715 2.286 565.9 25.2


PIPE SURROUND
5-Sep-17 15 7825 2.319 696.1 30.9

(16KM) KM 15 8015 2.375 652.5 29.0


13+028 RHS
15 7915 2.345 679.1 30.2

AVERAGE ( COMPRESSIVE STRENGTH ) 26.1 30.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

7-Aug-17 14-Aug-17 C20 190 15 7815 2.316 564.3 25.1


PIPE CULVERT
15 7960 2.359 578.0 25.7

15 7905 2.342 520.1 23.1


PIPE SURROUND
4-Sep-17 15 7973 2.362 625.3 27.8

(16KM) KM 15 8080 2.394 662.8 29.5


13+028 RHS
15 7930 2.350 682.2 30.3

AVERAGE ( COMPRESSIVE STRENGTH ) 24.6 29.2

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

7-Aug-17 14-Aug-17 C20 80 15 7980 2.364 602.9 26.8


PIPE CULVERT
15 7935 2.351 666.7 29.6

15 7835 2.321 601.4 26.7


PIPE SURROUND
4-Sep-17 15 7935 2.351 792.1 35.2

(16KM) KM 15 7945 2.354 794.0 35.3


13+028 RHS
15 7940 2.353 776.1 34.5

AVERAGE ( COMPRESSIVE STRENGTH ) 27.7 35.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer

FISH TOWN - HARPER ROAD PROJECT PHASE 1


Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

7-Aug-17 14-Aug-17 C20 100 15 7936 2.351 532.7 23.7


PIPE CULVERT
15 7946 2.354 539.7 24.0

15 7903 2.342 554.1 24.6


PIPE SURROUND
4-Sep-17 15 7905 2.342 646.2 28.7

(16KM) KM 15 7865 2.330 651.1 28.9


13+028 RHS
15 7845 2.324 631.7 28.1

AVERAGE ( COMPRESSIVE STRENGTH ) 24.1 28.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

7-Aug-17 14-Aug-17 C20 100 15 7815 2.316 664.3 29.5


PIPE CULVERT
15 7960 2.359 674.0 30.0

15 7905 2.342 620.1 27.6


PIPE SURROUND
4-Sep-17 15 7940 2.353 708.1 31.5

(16KM) KM 15 7945 2.354 702.7 31.2


13+028 RHS
15 7855 2.327 713.3 31.7

AVERAGE ( COMPRESSIVE STRENGTH ) 29.0 31.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

5-Sep-17 12-Sep-17 C30 60 15 7815 2.316 664.3 29.5


PIPE CULVERT
15 7960 2.359 674.0 30.0

15 7905 2.342 620.1 27.6


HEADWALL
3-Oct-17 15 7905 2.342 811.1 36.0

(16KM) KM 15 7980 2.364 778.2 34.6


13+028 RHS
15 7900 2.341 805.3 35.8

AVERAGE ( COMPRESSIVE STRENGTH ) 29.0 35.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

1-Aug-17 8-Aug-17 C15 140 15 7735 2.292 590.1 26.2


PIPE CULVERT
15 7690 2.279 606.3 26.9

15 7715 2.286 641.3 28.5


BLINDING
29-Aug-17 15 7735 2.292 765.9 34.0

(16KM) KM 15 7654 2.268 783.3 34.8


13+376 RHS
15 7750 2.296 747.0 33.2

AVERAGE ( COMPRESSIVE STRENGTH ) 27.2 34.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

1-Aug-18 8-Aug-18 C3- 140 15 7735 2.292 590.1 26.2


PIPE CULVERT
15 7690 2.279 606.3 26.9

15 7715 2.286 541.8 24.1


BASE
29-Aug-18 15 7875 2.333 759.1 33.7

(16KM) KM 15 7796 2.310 785.5 34.9


13+376 RHS
15 7835 2.321 722.1 32.1

AVERAGE ( COMPRESSIVE STRENGTH ) 25.8 33.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

10-Aug-17 17-Aug-17 C20 130 15 7984 2.366 635.0 28.2


PIPE CULVERT
15 8062 2.389 661.4 29.4

15 7998 2.370 678.4 30.2


PIPE SURROUND
7-Sep-17 15 7980 2.364 829.2 36.9

(16KM) KM 15 8050 2.385 787.4 35.0


13+376 RHS
15 8055 2.387 749.7 33.3

AVERAGE ( COMPRESSIVE STRENGTH ) 29.3 35.1

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

10-Aug-17 17-Aug-17 C20 110 15 7982 2.365 612.7 27.2


PIPE CULVERT
15 7958 2.358 570.7 25.4

15 7823 2.318 550.3 24.5


PIPE SURROUND
7-Sep-17 15 7960 2.359 593.6 26.4

(16KM) KM 15 7940 2.353 606.3 26.9


13+376 RHS
15 7870 2.332 605.5 26.9

AVERAGE ( COMPRESSIVE STRENGTH ) 25.7 26.7

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Aug-17 25-Aug-17 C30 100 15 8010 2.373 556.5 24.7


PIPE CULVERT
15 8065 2.390 669.0 29.7

15 8035 2.381 663.0 29.5


BLINDING
15-Sep-17 15 7850 2.326 557.4 24.8

(16KM) KM 15 8033 2.380 641.9 28.5


13+460 LHS
15 7845 2.324 556.9 24.8

AVERAGE ( COMPRESSIVE STRENGTH ) 28.0 26.0

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Aug-17 25-Aug-17 C30 100 15 8010 2.373 556.5 24.7


PIPE CULVERT
15 8065 2.390 669.0 29.7

15 8035 2.381 663.0 29.5


BASE
15-Sep-17 15 7850 2.326 557.4 24.8

(16KM) KM 15 8033 2.380 641.9 28.5


13+460 LHS
15 7845 2.324 556.9 24.8

AVERAGE ( COMPRESSIVE STRENGTH ) 28.0 26.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

21-Aug-17 28-Aug-17 C20 100 15 7995 2.369 667.3 29.7


PIPE CULVERT
15 7923 2.348 696.6 31.0

15 7845 2.324 624.7 27.8


PIPE SURROUND
18-Sep-17 15 8120 2.406 796.7 35.4

(16KM) KM 15 8120 2.406 818.5 36.4


13+460 LHS
15 8190 2.427 825.0 36.7

AVERAGE ( COMPRESSIVE STRENGTH ) 29.5 36.2

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

21-Aug-17 28-Aug-17 C20 100 15 8050 2.385 599.1 26.6


PIPE CULVERT
15 7950 2.356 606.7 27.0

15 7880 2.335 579.8 25.8


PIPE SURROUND
18-Sep-17 15 7965 2.360 657.7 29.2

(16KM) KM 15 7930 2.350 747.4 33.2


13+460 LHS
15 7960 2.359 607.6 27.0

AVERAGE ( COMPRESSIVE STRENGTH ) 26.5 29.8

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

21-Aug-17 28-Aug-17 C20 100 15 7995 2.369 607.3 27.0


PIPE CULVERT
15 7923 2.348 596.6 26.5

15 7845 2.324 624.7 27.8


PIPE SURROUND
18-Sep-17 15 7965 2.360 657.7 29.2

(16KM) KM 15 7930 2.350 747.4 33.2


13+460 LHS
15 7960 2.359 607.6 27.0

AVERAGE ( COMPRESSIVE STRENGTH ) 27.1 29.8

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

22-Aug-17 29-Aug-17 C30 150 15 7930 2.350 745.6 33.1


PIPE CULVERT
15 7850 2.326 808.5 35.9

15 7910 2.344 729.5 32.4


APRON
19-Sep-17 15 7975 2.363 825.0 36.7

(16KM) KM 15 7825 2.319 944.2 42.0


13+460 LHS
15 7725 2.289 936.8 41.6

AVERAGE ( COMPRESSIVE STRENGTH ) 33.8 40.1

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

22-Aug-17 29-Aug-17 C30 150 15 7880 2.335 688.2 30.6


PIPE CULVERT
15 7900 2.341 637.4 28.3

15 7885 2.336 612.4 27.2


TOE
19-Sep-17 15 7880 2.335 828.6 36.8

(16KM) KM 15 7900 2.341 857.8 38.1


13+460 LHS
15 7885 2.336 814.5 36.2

AVERAGE ( COMPRESSIVE STRENGTH ) 28.7 37.1

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Sep-17 19-Sep-17 C30 140 15 7720 2.287 632.1 28.1


PIPE CULVERT
15 7925 2.348 557.1 24.8

15 7935 2.351 701.9 31.2


WING WALL
10-Oct-17 15 7840 2.323 754.7 33.5

(16KM) KM 15 7960 2.359 744.1 33.1


13+460 LHS
15 7980 2.364 669.3 29.7

AVERAGE ( COMPRESSIVE STRENGTH ) 28.0 32.1

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Aug-17 19-Aug-17 C30 130 15 8049 2.385 723.1 32.1


PIPE CULVERT
15 8165 2.419 756.2 33.6

15 7986 2.366 780.6 34.7


TOE & APRON
9-Sep-17 15 8080 2.394 910.8 40.5

(16KM) KM 15 8090 2.397 805.7 35.8


13+860 LHS
15 8030 2.379 936.9 41.6

AVERAGE ( COMPRESSIVE STRENGTH ) 33.5 39.3

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Aug-17 19-Aug-17 C15 130 15 8049 2.385 723.1 32.1


PIPE CULVERT
15 8165 2.419 756.2 33.6

15 7986 2.366 780.6 34.7


BLINDING
9-Sep-17 15 8080 2.394 910.8 40.5

(16KM) KM 15 8090 2.397 805.7 35.8


13+860 LHS
15 8030 2.379 936.9 41.6

AVERAGE ( COMPRESSIVE STRENGTH ) 33.5 39.3

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Aug-17 19-Aug-17 C30 130 15 8049 2.385 723.1 32.1


PIPE CULVERT
15 8165 2.419 756.2 33.6

15 7986 2.366 780.6 34.7


BASE
9-Sep-17 15 8080 2.394 910.8 40.5

(16KM) KM 15 8090 2.397 805.7 35.8


13+860 LHS
15 8030 2.379 936.9 41.6

AVERAGE ( COMPRESSIVE STRENGTH ) 33.5 39.3

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Aug-17 25-Aug-17 C20 90 15 7955 2.357 567.1 25.2


PIPE CULVERT
15 7900 2.341 626.4 27.8

15 7975 2.363 605.6 26.9


PIPE SURROUND
15-Sep-17 15 7850 2.326 557.4 24.8

(16KM) KM 15 8033 2.380 641.9 28.5


13+860 LHS
15 7845 2.324 556.9 24.8

AVERAGE ( COMPRESSIVE STRENGTH ) 26.7 26.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

18-Aug-17 25-Aug-17 C30 90 15 7930 2.350 745.6 33.1


PIPE CULVERT
15 7850 2.326 808.5 35.9

15 7910 2.344 729.5 32.4


PIPE SURROUND
15-Sep-17 15 7850 2.326 557.4 24.8

(16KM) KM 15 8033 2.380 641.9 28.5


13+860 LHS
15 7845 2.324 556.9 24.8

AVERAGE ( COMPRESSIVE STRENGTH ) 33.8 26.0

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

5-Sep-17 12-Sep-17 C30 60 15 7815 2.316 664.3 29.5


PIPE CULVERT
15 7960 2.359 674.0 30.0

15 7905 2.342 620.1 27.6


WING WALL
3-Oct-17 15 7905 2.342 811.1 36.0

(16KM) KM 15 7980 2.364 778.2 34.6


13+860 RHS
15 7900 2.341 805.3 35.8

AVERAGE ( COMPRESSIVE STRENGTH ) 29.0 35.5

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

8-Aug-17 15-Aug-17 C15 80 15 8015 2.375 576.4 25.6


PIPE CULVERT
15 7875 2.333 516.6 23.0

15 7990 2.367 542.2 24.1


BLINDING
5-Sep-17 15 8060 2.388 879.4 39.1

(16KM) KM 15 7965 2.360 752.6 33.4


14+160 LHS
15 7960 2.359 660.0 29.3

AVERAGE ( COMPRESSIVE STRENGTH ) 24.2 34.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

8-Aug-17 15-Aug-17 C30 80 15 8015 2.375 576.4 25.6


PIPE CULVERT
15 7875 2.333 516.6 23.0

15 7990 2.367 542.2 24.1


BASE
5-Sep-17 15 8060 2.388 879.4 39.1

(16KM) KM 15 7965 2.360 752.6 33.4


14+160 LHS
15 7960 2.359 660.0 29.3

AVERAGE ( COMPRESSIVE STRENGTH ) 24.2 34.0

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Aug-17 19-Aug-17 C20 70 15 8125 2.407 647.5 28.8


PIPE CULVERT
15 8045 2.384 586.3 26.1

15 8090 2.397 535.3 23.8


PIPE SURROUND
9-Sep-17 15 8355 2.476 709.5 31.5

(16KM) KM 15 8295 2.458 788.2 35.0


14+160 LHS
15 8180 2.424 758.9 33.7

AVERAGE ( COMPRESSIVE STRENGTH ) 26.2 33.4

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Aug-17 19-Aug-17 C20 70 15 8125 2.407 647.5 28.8


PIPE CULVERT
15 8045 2.384 586.3 26.1

15 8090 2.397 535.3 23.8


PIPE SURROUND
9-Sep-17 15 8105 2.401 743.8 33.1

(16KM) KM 15 8170 2.421 791.7 35.2


14+160 LHS
15 8080 2.394 674.4 30.0

AVERAGE ( COMPRESSIVE STRENGTH ) 26.2 32.7

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

5-Sep-17 12-Sep-17 C30 60 15 7815 2.316 664.3 29.5


PIPE CULVERT
15 7960 2.359 674.0 30.0

15 7905 2.342 620.1 27.6


WING WALL
3-Oct-17 15 7905 2.342 811.1 36.0

(16KM) KM 15 7980 2.364 778.2 34.6


14+160 RHS
15 7900 2.341 805.3 35.8

AVERAGE ( COMPRESSIVE STRENGTH ) 29.0 35.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

7-Sep-17 14-Sep-17 C30 80 15 7835 2.321 625.9 27.8


PIPE CULVERT
15 7910 2.344 539.5 24.0

15 7995 2.369 610.3 27.1


TOE & APRON
5-Oct-17 15 8035 2.381 777.1 34.5

(16KM) KM 15 8035 2.381 752.2 33.4


14+274 LHS
15 8027 2.378 784.2 34.9

AVERAGE ( COMPRESSIVE STRENGTH ) 26.3 34.3

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

14-Sep-17 21-Sep-17 C30 110 15 7835 2.321 625.9 27.8


PIPE CULVERT
15 7910 2.344 539.5 24.0

15 7995 2.369 610.3 27.1


TOE & APRON
12-Oct-17 15 7835 2.321 725.7 32.3

(16KM) KM 15 7910 2.344 739.5 32.9


14+274 LHS
15 7995 2.369 710.5 31.6

AVERAGE ( COMPRESSIVE STRENGTH ) 26.3 32.2

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

20-Aug-17 27-Aug-17 C15 80 15 7850 2.326 616.5 27.4


PIPE CULVERT
15 7745 2.295 624.3 27.7

15 7850 2.326 637.0 28.3


BLINDING
17-Sep-17 15 7770 2.302 674.6 30.0

(16KM) KM 15 7800 2.311 691.3 30.7


14+560 RHS
15 7885 2.336 764.3 34.0

AVERAGE ( COMPRESSIVE STRENGTH ) 27.8 31.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

20-Aug-17 27-Aug-17 C30 80 15 7850 2.326 616.5 27.4


PIPE CULVERT
15 7745 2.295 624.3 27.7

15 7850 2.326 637.0 28.3


BASE
17-Sep-17 15 7770 2.302 674.6 30.0

(16KM) KM 15 7800 2.311 691.3 30.7


14+560 RHS
15 7885 2.336 764.3 34.0

AVERAGE ( COMPRESSIVE STRENGTH ) 27.8 31.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

25-Aug-17 1-Sep-17 C20 80 15 8045 2.384 599.6 26.6


PIPE CULVERT
15 7950 2.356 596.4 26.5

15 7955 2.357 516.0 22.9


PIPE SURROUND
22-Sep-17 15 7995 2.369 666.8 29.6

(16KM) KM 15 7995 2.369 685.3 30.5


14+560 RHS
15 7950 2.356 570.4 25.4

AVERAGE ( COMPRESSIVE STRENGTH ) 25.4 28.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Sep-17 19-Sep-17 C30 120 15 7850 2.326 616.5 27.4


PIPE CULVERT
15 7745 2.295 624.3 27.7

15 7850 2.326 637.0 28.3


BLINDING
10-Oct-17 15 7770 2.302 674.6 30.0

(16KM) KM 15 7800 2.311 691.3 30.7


14+560 RHS
15 7885 2.336 764.3 34.0

AVERAGE ( COMPRESSIVE STRENGTH ) 27.8 31.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Sep-17 19-Sep-17 C30 120 15 7850 2.326 616.5 27.4


PIPE CULVERT
15 7745 2.295 624.3 27.7

15 7850 2.326 637.0 28.3


BASE
10-Oct-17 15 7770 2.302 674.6 30.0

(16KM) KM 15 7800 2.311 691.3 30.7


14+560 RHS
15 7885 2.336 764.3 34.0

AVERAGE ( COMPRESSIVE STRENGTH ) 27.8 31.6

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Sep-17 19-Sep-17 C30 140 15 7720 2.287 632.1 28.1


PIPE CULVERT
15 7925 2.348 557.1 24.8

15 7935 2.351 701.9 31.2


WING WALL
10-Oct-17 15 7840 2.323 754.7 33.5

(16KM) KM 15 7960 2.359 744.1 33.1


14+560 RHS
15 7980 2.364 669.3 29.7

AVERAGE ( COMPRESSIVE STRENGTH ) 28.0 32.1

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

12-Sep-17 19-Sep-17 C30 140 15 7720 2.287 632.1 28.1


PIPE CULVERT
15 7925 2.348 557.1 24.8

15 7935 2.351 701.9 31.2


WING WALL
10-Oct-17 15 7840 2.323 754.7 33.5

(16KM) KM 15 7960 2.359 744.1 33.1


14+723 RHS
15 7980 2.364 669.3 29.7

AVERAGE ( COMPRESSIVE STRENGTH ) 28.0 32.1

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

25-Aug-17 1-Sep-17 C30 180 15 7735 2.292 660.2 29.3


PIPE CULVERT
15 7590 2.249 559.1 24.8

15 7775 2.304 594.0 26.4


BASE
22-Sep-17 15 7790 2.308 781.4 34.7

(16KM) KM 15 7755 2.298 704.5 31.3


15+175 RHS
15 7745 2.295 632.8 28.1

AVERAGE ( COMPRESSIVE STRENGTH ) 26.9 31.4

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

25-Aug-17 1-Sep-17 C15 180 15 7735 2.292 660.2 29.3


PIPE CULVERT
15 7590 2.249 559.1 24.8

15 7775 2.304 594.0 26.4


BLINDING
22-Sep-17 15 7790 2.308 781.4 34.7

(16KM) KM 15 7755 2.298 704.5 31.3


15+175 RHS
15 7745 2.295 632.8 28.1

AVERAGE ( COMPRESSIVE STRENGTH ) 26.9 31.4

Remarks:

Contractor's Materials Engineer Checked By Materials Engineer


FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

30-Aug-17 6-Sep-17 C30 60 15 7750 2.296 454.6 20.2


PIPE CULVERT
15 7770 2.302 536.9 23.9

15 7720 2.287 534.3 23.7


PIPE SUROUND
27-Sep-17 15 7710 2.284 562.4 25.0

(16KM) KM 15 7807 2.313 665.1 29.6


15+175 RHS
15 7780 2.305 621.6 27.6

AVERAGE ( COMPRESSIVE STRENGTH ) 22.6 27.4

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer
FISH TOWN - HARPER ROAD PROJECT PHASE 1
Paving of Harper - Karloken (50km) and Maintenance of Karloken to Fish Town
(80km)

Structure Date Concrete Slump Cube Weight Density Failure Load (kN)
Compressive
and Location Cast Crush Class size of Cube Strength (N/mm2)
of Cube
(mm) (cm3) (kg) (g/cm3) 7/day 28/days 7/day 28/days

28-Aug-17 4-Sep-17 C30 150 15 7900 2.341 636.6 28.3


PIPE CULVERT
15 7805 2.313 559.2 24.9

15 8010 2.373 596.7 26.5


BASE
25-Sep-17 15 7805 2.313 752.4 33.4

(16KM) KM 15 7925 2.348 795.6 35.4


15+175 RHS
15 7865 2.330 710.0 31.6

AVERAGE ( COMPRESSIVE STRENGTH ) 26.6 33.5

Remarks:
Contractor's Materials Engineer Checked By Materials Engineer