Вы находитесь на странице: 1из 1

'-r::-I Advanced TCR ADVANCED ENGINEERING PVT. LTD.

IL" Engineering P.ltd.


Research Center & Testing Division:
Regd. Off. : 250·252/9, GrOC Estate, Makarpura, Vadodara - 390010

Managing Director
PH: (0265) 2657233, 7574805594,7574805595,8511117993
Paresh U. Haribhakti Email: testing@tcradvanced.com Website: www.tcradvanced.com
BE. (MeL). M.E. (Mal. Tech.) MIE.
LMIIM,LMIIW, Chartered Engineer ON APPROVED LIST OF VARIOUS GOVT. DEPARTMENTS AND PUBLIC SECTOR UNDERTAKINGS
TC -6739

TEST REPORT
Report No: R-03107.1
To, _ _.._-- I ULR - TC673919000002457F I Date: 01/02/2019
J Page 1 of 1

lA.V.STEEL FORGINGS PVT. LTO.


IPlot No - 25,Savli GJ_DC
Estate,Village-Ma~j_~~~!,Tal:Savli Dist -_,{?dodara -._
-
I~EST: Tensile Test
ItrEST METHOD: EN ISO 6892·2016
iTest Performed at: TCR Advanced Engineering Pvt. l.td., Testing Division
- ---- - - -.
Instrument Utilized: 0-40T, TCRADV/E-2
i*Customer's Reference: Ch No-AVS/0336, Dated: 28.01.2019
Sample received on: 28/01/2019
*Condition of sample: Test Piece - 202 mmDia
...:.--.-----.------------- ..'-
Specification: EN 10083-1 Grade 30CrNiMo8
Date of completion of test: 31/01/2019
- ---~.- - ~~--. j_
Sample Drawn by: Iparty
PLE ID: Heat No - K18-1313, Hardened - Tempered Condition, Punch As AVS, (Ruling section 160
mm < D < 250 mm ))
TEST RESULT REQUIRED
IGauge Dia. (mm) 10.07
IArea (rnrn") 79.64
Gauge Length (mm) 50.00
Final Length (mm) 58.05
Final Dia. (mm) 6.34
Yield Load (N) 69040
Ultimate Load (N) 78360
Yield Stress (N/mm2) 867.00 700 Min
UTS (N/mm2) 984.00 900 - 1100
% Reduction in area 60.36 50 Min
% Elongation 16.11 12 Min
Fracture W.G.L
Remarks: Result meets the tensile requirements of EN':1~083-1Grade 30CrNiM08.
End of report.

Checked By:Umang ignatory