OBTAINING THE LIGHT GASOLINE FRACTIONS AND OLEFINS BY
CATALYTIC CRACKING OF THE OIL PARAFFINCONTAINING HEAVY
RESIDUE
Sedghe Rouhi Babak, Kapustin .V. F , Tretyakov . V.F. Gerzeliyev.I.M.
Abctract
The primary purpose is the new approach to the development of deep processing of
oil stimulated by the energy strategy of Russia . Heavy oil residues are converted at low
temperatures into fuel products . The goal of the developed technology ,is to provide the
conversion of the heavy residue fractions for the subsequent processing by the catalytic
cracking (FCC) into light olefins and gasoline.
Key words: Catalytic Cracking (FCC), Gasoline ,Propylene ,isobutane.


, [1,2],
[3] .

(), .
CH
( 400 /).

,
.
.
,
,
, ,
.
,
.

(- () [4,5]). ,

( .) ,

1-4 ,
.

()

( 60%), (8%) (4%).


(~ 0,1%).
()
( 1-4) (.1) 1
80 520-580C,
5-30C ,
0,3-1,2% .
15-25C .
1-4, ,


330C, 3.

,
.

.1. - .
1 ; 2 ; 3,5
; 4 ; 6 ; 7
.
1
2, 500-540C.
() -
Finnigan MAT 95XL ( Varian VF-5ms, 30 ,
0.25 , 0.25 , - , :
270, - 30,
5 10/ 300).

-,

NIST/EPA/NIH 08.

.

7-22 , ,
(.2). ,
, , 5-6 .

n-C11
RT: 0.00 - 25.82
NL:
1.30E7
m/z=
20-27+
29-31+
33-39+
41-43+
45-800 MS
anzor13957

11.25

100
95
90

n-C13

85

13.31

80
75

n-C16

70

n-C9

Relative Abundance

65

n-C19

15.86

8.51

18.05

14.22 15.07

60
17.35
55

16.62

10.03

n-C22

50
12.34

n-C8

45

19.93

6.43

40

19.32

20.50

35
21.08

30
25

n-C7

20

3.52

8.39

18.69
22.14

9.06
7.30

15

8.00
3.37

10

1.68 2.10
2.17
1.38
2.89
0.71

5
0
0

6.21

4.13

22.62
23.13
24.07

5.46
4.85
4

10

12
14
Time (min)

16

18

20

22

24

. 2.
()
, ,
.
,


-
.
, ,

:
, [6].

RD-DMS-PM, -
. 1.

500
7 -1 .
.2. .2
,
2 (.1).
1. - RDDMS-PM.


:



()

()
20-40
40-80
80-105
105-149
( Engelhard)

/3

2/
/3

91
0,25
10,1

. %
. %
. %
. %

40,6
0,16
0,55
1,07

. %
. %
. %
. %

2
52
30
11
54

0,97

.
PLOT- HPPLOT/Q ( Varian),
, 2 H2S. ,
,
(N2, O2, , 4).
.

,
DB-2887 ( Varian) (L=30 , D=0,53 ) -
.
. 2 .3.


, %
, :
13,7
, ..
2,9
- , ..
4,4
-
3,2
- , ..
6,5

()
14,3
1
5,7
4,1
7,7

2.

-
-
(-200 )
(200-320)
(320+)
+

3,5
2,5
43
19
19,3
5

1,2
5,9
49
21.5
9
6,2


, ,
( 1-4)
.

,

,

(. .2) ,

50
40
30

20

10

60

7
6
5
4
3
2
1
0


(320+)

. 3.


.


1. . ., . ., . . .
: , 1997.
2. . ., . ., . . // . 2002. . 42.
3. . 195.
3. . . // . 1998. 8. . 42.
4. Lucchesi P. T., Tarmy B. L., Long R. B. et al. // Industrial Engineering Chem. 1958.
V. 50. 6. P. 879.
5. Zaykina R. F., Zaykin Yu. A., Mamedova T. V. et al. // Radiat. Phys. Chem. 2001.
V. 60. P. 211.
6... , .X. , .. ,
: /. . .. . .:
, 2009. 832 : .

Вам также может понравиться